The heat resistance of FeCrAl, FeCrNi and CrNi alloys is shown in this table. The temperature limits listed, °C/°F, are those temperatures where the protecting oxide starts to fall off-the scaling temperature. Even if the materials can be used at these temperatures, use at lower temperatures prolonges the service life.
Kanthal APM is manufactured using powder metallurgy, hence the improved hot strength as compared to the other FeCrAl alloys.

Exothermic gas: 10CO, 15H2, 5CO2, 70N2

Properties/Ranking Less good Good Very good Better Best
Hot strength, T>600C/1112F Kanthal D
Tp 446
Kanthal AF Alloy 600 Tp 310 Kanthal APM Alloy 800HT 253MA Alloy 601
Oxidation resistance in dry air Tp 309, 1050°C/1922F Alloy 800HT, 1050°C/1922F Tp 446, 1100°C/2012F Alloy 600, 1100°C/2012F 253MA, 1150°C/2102F Alloy 601, 1150°C/2102F Tp 310, 1150°C/2102F   Kanthal APM, 1425°C/2600F Kanthal AF, 1300°C/2372F Kanthal D,1300°C/2372F
Oxidation resistance in moist air Tp 309, 900°C/1652F Alloy 800HT, 900°C/1652F Tp 446, 950°C/1752F Alloy 600, 950°C/1752F 253MA, 1000°C/1832F Alloy 601, 1000°C/1832F Tp 310, 1000°C/1832F   Kanthal APM, 1200°C/2192F Kanthal AF, 1200°C/2192F Kanthal D, 1200°C/2192F
N2, nitrogen from an oxygen plant Tp 446, 650°C/1202F Tp 309, 650°C/1202F 253MA, 750°C/1382F Tp 310, 800°C/1382F Alloy 600, 1000°C/1832F Alloy 601, 1000°C/1832F Alloy 800HT, 900°C/1652F Kanthal APM, 1050°C/1922F Kanthal AF, 1100°C/2012F Kanthal D, 1000°C/1832F Not preoxidized Kanthal APM ,1200°C/2192F Kanthal AF, 1200°C/2192F Kanthal D, 1200°C/2192F Preoxidized
Ar, Argon Tp 446, 950°C/1752F Alloy 800HT, 950°C/1752F Alloy 600, 950°C/1752F 253MA, 1000°C/1832F Alloy 601, 1000°C/1832F Tp 310, 1000°C/1832F     Kanthal APM, 1425°C/2600F Kanthal AF, 1300°C/2372F Kanthal D, 1300°C/2372F
Tp 446 253MA, 850°C/1562F Tp 310, 850°C/1562F Alloy 800HT, 950°C/1752F Alloy 601, 1000°C/1832F Alloy 600, 1000°C/1832F Kanthal APM, 1150°C/2102F Kanthal AF, 1150°C/2102F Kanthal D, 1100°C/2012F  
Endothermic gas: 20CO, 40H2, 40N2 Tp 446 253MA, 700°C/1292F Tp 310, 750°C/1382F Alloy 601, 900°C/1652F Alloy 600, 900°C/1652F Alloy 800HT, 800°C/1472F Kanthal D, 1000°C/1832F Kanthal APM, 1050°C/1922F Kanthal AF, 1050°C/1922F
H2, hydrogen, dewpoint<-50 Tp 446, 900°C/1652F 253MA, 1000°C/1832F Alloy 800HT, 1000°C     Kanthal APM, 1425°C/2600F Kanthal AF, 1400°C/2552F Kanthal D, 1300°C/2372F
Vacuum, 10-3 torr         Kanthal APM, 1150°C/1922F Kanthal AF, 1200°C/2192F Kanthal D, 1100°C/2012F
Oxidizing SO2, SO3-containing gas*   Alloy 800HT, 600°C/1112F 253MA, 900°C/1652F Tp 446, 950°C/1752F Tp 310, 950°C/1752F   Kanthal APM, 1200°C/2192F Kanthal AF, 1200°C/2192F Kanthal D, 1150°C/2012F
Reducing sulfur containing gas   253MA, 650°C/1202F Alloy 800HT, 600°C/1112F Tp 310, 650°C/1202F Tp 446, 700°C/1292F   Kanthal APM, 1025°C/1877F Kanthal AF, 1025°C/1877F Kanthal D, 1000°C/1832F
Molten metals; Cu**, Zn, Mg   253MA

Tp446

Kanthal APM, AF  
Molten aluminum Metallic materials dissolve!        
Cracked ammonia     253MA, 750°C/1382F SS2361, 800°C/1382F Alloy 800HT, 900°C/1652F Kanthal APM, 900°C/1652F Kanthal AF, 900°C/1652F Kanthal D, 900°C/1652F Alloy 601, 1000°C/1832F Alloy 600, 1000°C/1832F

KANTHAL is a registered trademark of Kanthal AB;
253MA is a registered trademark of AvestaPolarit AB.

* Under deposits, conditions may be reducing
** Nickel containing alloys are rapidly attacked